Strength Evaluation Techniques that Help Improve Accuracy of CAE Analysis for Composite Materials
—In-Plane and Out-of-Plane Shear Properties of CFRTP—

The use of carbon fiber reinforced thermoplastic (CFRTP) composites, which have higher specific strength than conventional materials and excellent processing and forming properties, is being considered as structural materials in automobiles, where strength and durability are required.
Unlike isotropic conventional materials, composite materials such as CFRTPs are anisotropic and exhibit complex failure behavior in tension, compression, bending, in-plane shear, and out-of-plane shear tests, or a combination of these, depending on the principal axes of stress when loaded. When performing testing and evaluation with a view to designing products using CAE analysis, there is a strong need for testing methods that enable genuine evaluation of these failure behaviors. Here we introduce an example of using a testing system that can evaluate the in-plane and out-of-plane shear properties of composite materials to evaluate one type of CFRTP, namely chopped tape randomly laminated material (CTT, polypropylene base).

In-Plane Shear Test —Evaluation of Local Strain Dependence Using a Virtual Strain Gauge (DIC Analysis)—

Test Sample Shape, Strain Gauge Installation Position, and Random Mark Coated Part

Test Sample Shape, Strain Gauge Installation Position, and Random Mark Coated Part

Evaluation of the Correlation between the Failure Image and the Stress-Stroke Graph

Evaluation of the Correlation between the Failure Image and the Stress-Stroke Graph

Local Strain Evaluation(Comparison of Virtual Strain Gauge and Strain Gauge)

Local Strain Evaluation
(Comparison of Virtual Strain Gauge and Strain Gauge)

  • In-plane shear testing in accordance with ASTM D7078 can be performed using strain gauge measurement (4 ch).
  • In-plane distribution can be evaluated by DIC analysis, and multi-point strain measurement can be evaluated with virtual strain gauges.

Out-Of-Plane Shear Testing
—Development of a New Testing Method Using CAE Analysis—

Dependence of Out-Of-Plane Strain Distribution on Test Sample Shape (CAE Analysis)

Dependence of Out-Of-Plane Strain Distribution on Test Sample Shape (CAE Analysis)

Test Sample Fixing Jigs and Parallelism Adjustment

Test Sample Fixing Jigs and Parallelism Adjustment Plates

A-3, which had the lowest shear properties and where shear failure only occurred, is the ideal test sample shape.

A-3, which had the lowest shear properties and where shear failure only occurred, is the ideal test sample shape.

  • The linear and non-linear behavior of out-of-plane shear samples, which was previously difficult to measure, can be evaluated experimentally.

Acknowledgments
A part of this research was performed as part of the Japanese Ministry of Economy, Trade and Industry—NEDO sponsored project “Research and Development of Innovative Structural Materials,” and we are grateful to all those that were involved.